Post on 05-Jul-2018
� � � �� � � � � � � �
���� ���������� ��
���
····················
terials and test,mmondefor-essure was, the
····················
····················
������ �� ��� ��� ���� ������
��������� ��������� �������������� � ��� ��� ������� �� ������� ���� �����
����������
Jeon, Joo-Yong�Lee, Kwan-Ho
·········································································································································································································
Abstract
The purpose of this research was to evaluate and suggest the permanent deformation properties of asphalt paving mawith recycled waste materials, like waste foundry sand and various slags. Couple of laboratory tests with various loadingsconfining pressure were conducted on for evaluation of permanent deformation of hot mix asphalt. Judging from the creephot mix asphalt with steel slag or furnace slag as coarse aggregates showed the lower permanent deformation than coaggregates. Those were reduced up to more than 50% of permanent deformation of hot mix asphalt. The permanent mation by static creep test was lower than by repeated creep test. Type of loading, testing temperature, and confining prshould be considered as important factors for evaluation of permanent deformation of hot mix asphalt. VESYS methodemployed and its results were similar to static or repeated creep tests. From the prediction of rutting potential by VESYSsteel slag mixtures showed better performance than the common aggregate mixtures.
Keywords : waste foundry sand, slag, recycled mateials, rutting, creep, VESYS
·········································································································································································································
� �
� ��� ���� �� ������ ��� ���� � ���� ��� �� !"#$ �� % &��'�( %& �)*+ ,-�� ./0 1234, %� !" 56� �0 7& 8��9( :;3� <%=. .>, ?@ �)*+ ,-�� ABC� DEFG� H/IF./0 1234, H/IF� JK/% L ��'�( �&�)*+ ,-�0 :;34� &=. ��'�( %& �)*+ ,-� ;MN �" H/IF./12� �OP0 Q4,=R& �S(T3U/V3U, W�X/�XYZ)� [\];M0 %3^=. [\];M _� :`��� � 4"��� '�(%& �)*+ ,-�� H/IF% �a'� ,-�� Wb c 50% %d ef ghi=. j&, T3U [\];M� Wb V3U[\] ;M; ;k� H/IFT!2 lm [f ghi4, %( 8n" op, H/IF 12( 7b � V3U,4q(40!%d) � �X3U0 %& ;M0 %3� <% rstu <v" wxy=. j&, �)*+ ,-�� H/IF./0 1238 7b VESYS� zM{|( C3} [\];M0 ~�3^4, %( %& b�_�, ��'��0 %& �)*+ ,-�� �� H/IF% �a'�( %& �)*+ ,-�� Wb dACv" ef ghi=. .>, :`���( %& ,-�N H/IF �H� d�& ��2 ��0 ��3^=.
���� : ����, ���, ��'�, H/IF, [\];M, VESYS
·········································································································································································································
1. ���� � ��
������ 1998� 12� � �� �� ���
���� � 90,000km��, ���� ���� � 75%�
�� . �!�� " #$��, %&'�(� )* ����
�� � 95%��� . ����+, -.� 1993��/ 0
� � 30%�� 12�3�, 1998� 456� � 778 �
�2 ����-.6� 9:;< . => ?@ 10�A� �
�� ��+, �-.� � 10078 �B� C D6� E
��� F . ��G H IJB K4 ��L� LM� 0N
OPQ, 'A� PR� ST U@;G ��� VP+WL &
' OX 12�� FG EY� . 1997� ��� � �
� ?@ 10�A ��� VPZ[� \];G -.^ �
178 ��� E.�� F . _`ab ����� cd��
ef� 3c Vg�G hijg(permanent deformation), k
�*l(fatigue), mn*l(low temperature cracking)� F .
�� _`ab ��ef� op gqG hijg6� ��
ef� � 70%�B^ rP�� F�, U@p ��� op
ef� gq� k�*l &' Bs> �t^ rP�� F .
�u> ef� v�� wN ��9�x Vy��, 9z�6
�G ��� J{m�� �> |}L:^ 12'~�, =>
��x ��, VP +W�G o�� �� L:� 1cx 2
���������� ��� �� �������������� ��� �?�� ��, ��(khlee@ks.ac.kr)
�24� �2D� · 2004� 3� − 1 −
�n .
� �i��G ��:��(��H " �o|9)x �:>
_`ab ��|� \JjgIJ^ )2�4 �� �> 7
��� OW�'� [���, ���/ \JjgIJ -��
�]> j[�^ ��> . =>, ��p ��j[x �:�
� KENLAYER ��J ��H�^ �:> ��� ��^
[��� v� _`ab ��|� \JjgIJ )2��,
���6�G \Jjg� m J� ¡ ��:�� �: _
`ab ��|^ ¢'�G D� .
2. �� � �� ����
2.1 ������
OW� '�� _`ab ��|� \JjgIJ^ )2�
G 2� cd�� '�6� �M-jg+£� �> ��|�
¤�JIJ^ ¥¦§ (Hick, 1988; Khedr, 1986; van de
Loo, 1974; SHRP, 1994). �n��� _`ab ��|�
_`ab� ¤J� n�� 12� ST ¨©�X ª\�«
�, o� ��� ¬| ®B� �� ��|� IJ� ��
;�, �¯� °±� o� L²g°±IJ^ Z�5 . ST
�, ��|� IJ^ �³´ )2�4 ���G �MO4, '
A, n� (^ ¢µ��¶ �·, I´, i!¸�(confining
pressure)� �:��� ST, H IJ� OX j> . _`
ab2 2� ¹� w��G n�(10-50oC)c&��G 9:p
_`ab º�»� IJ� 0N ¼ª�X j> . Hu¥, �
�|� &½� IJ¾ j¿�G HW ¡ h?^ oP À�
G D6� ¥¦Á . �G ��|� IJ� 9:p ���
IJ� �> ?^ ¹� ÂG D^ �Ã> .
_`ab ��|� jgIJ� Ä ��� IJ)2Å
G ÆW #�> O4� �M� $Ç ���G ÈÉ^ �:
�·, �¯ yÊ�G jgIJ^ H 2.1Ë Ì� 42P ]
\, Í �J, \J, ¤�J " ¤\J h&6� it�� Î
[ F . �JjgË \Jjg� �M^ ��> DË ±'�
yÊ�G jgIJ6� �M��'AËG B+Ï . �� $
� ¤�J " ¤\J jg� Ì� O4� �M� P!Ð�
ST y�G 'A�� jg� . Uzan(1996)� �� ,
�n " ÒÄ �M��G \Jjg� o] ]\��, ¤\J
IJ� Bs´ ÃÃ� � yd�3 .
²g-¤�JIJ^ �:> _`ab ��|� IJ)2G
'�n� " �M��'A� ÓËx MÔ� 8Wx �:�
� _`ab ��|� �V> �M-jgIJ^ )2Õ [ F
G �¤^ 2Ö . �u> ²g-¤�J IJ^ ���G e
TÃ/G '�ÈÉ� ST creep modulusÅ relaxation
modulus, complex modulus, resilient modulus(MR)(6�
d®p . creep modulus, creep compliance " relaxation
modulus� ��G ×Ë Ì .
ØÙ�G _`ab ��|� °±IJ^ hi(\J)jgIJ
^ $h> ÚÛ^ vy�� �:�G EY� . �� cd�
� gq2 \J(plastic), �\J(Elasto-Plastic)Úg, ¤\J
(Visco-Plastic)Úg(� F . \J(plastic deformaion)� _
`ab ��|� ef =G ��|�� ��� ÜÝÞ (�
�� yÊ�G jg^ �Ã> . plastic flowG ¤J(visco)
IJ6� �� P!�� jg� Ê4G IJ^ �Ã> . �
u> \JjgIJ^ ßà�4�� iJÈ�á(constitutive
model)� �:;·, iJÈ�á� o] iJ]\G eâß5
(yield function), ãäIJ(flow rule) " w¿IJ(hardening
rule) (� F .
2.2 ����� �� ��
ØÙ� �� rå6� �> cd�� Iæ6�G cgrå
^ o] [ç[è6� �:�Gé� yÊ> . Í, ê�M�
12, ¦µµ ¸�� 12 " ��å� ¨!> 12x Z�
o� F . ST�, 'ë@ yÊ�G ��� \Jjg� c
> �³> -�� �[���, => �G Ë�> \Jjg6
� �> �� 9�� -� 0N M]> ]\� . \Jj
g� -��G ���� ì�-jg+£, rå�M� �> \
Jjgå (� �:;�, ��ÈÉ�G �í� ��É, &½
� ��É, w�^ Ù°�> &½� ��É (� F . \J
jg )2 " -�^ �� ®� Zî�6� 9:�G ÈÉ
6�G �jg�í =G ¤�J�í^ �:> ��É� .
\JjgË +,p ¹� �i2 ��ï�� [�;<�, =
> ¹� \Jjg mªcð� ¢ñ;< . �u> mªcð
� ÙA� òm \Jjg IJ^ �³´ )2�G D� .
I´, \Jjg� �³> -�^ �� 9:;G ÈÉ�¥
�í� oµÖ �M� �> ���� °±IJ^ �³´ )
2Õ [ Fµ¶��, => �� IJ^ �³´ $hÕ [
Fµ¶> . \Jjg IJ )2� �:;G ÈÉ� OX 3
2P� ¥óµ Î [ F . Í, zôt�^ �:> w��
ÈÉ, iJÈ�á^ �:> \Jjg �:É, õ��Ëx �
:> È�á6� it� Î [ F . �u> �> ��È
É^ �:> hijgIJ)2 �Ë, hijg� Bs> h
?^ oG ]\�G n�, �M$Çö[ " ��'A, ��
|IJ " ì�Bq (� F . #�t� ÚÛ� hijg
IJ )2' #ê¸êì�(σ1)Ë [)ì�(σ2)x �:�3 .
S t( )σ0
ε t( )--------=
D t( ) 1S t( )--------- ε t( )
σ0--------= =
Er t( ) σ t( )ε0
---------=
�� 2.1. �� �� ����� ��
− 2 − ����� �
�u> '�÷^ �:> ¹� �i�Ëx d 2.1� �W�
3 .
3. ����
3.1 ���
� �i��G ���� Zî�6� �:;� FG AP-3
Å AP-5 M P&� IJ, Í n¿> 4@x Z�G �.P
&^ �ø�� ��OO9� AP-5 _`ab 'ùb(AC,
Asphalt Cement)x ²ú�� õ�^ õ'�3 . � �i�
�:p _`ab� 4� |J¾G LM� 1.034 g/cm3, �
¿¤� 348oC, û� 150cm, ü�'� @ ý}|� 0.1%�
�� .
3.2 ��
� �i��G þ���� ¢ÿ��H " ����Hx �
:�3�, ý��� �o|9, ¢ÿ��H " ����Hx
�:�3 . 2l_`ab ��|: ����� IJ^ )2
�4 �� ��, LM " �[å'�, ±���� c> ñ�
J'�, ���Ú'�, Y�L'� ( õ'�3 . =>, #
$��x �:�� IJ^ )2�3�, � �i� 9:p �
Ê��� IJË B� L��3 . õ��ËG �o: (
(2002)� ��� yd�3 .
3.3 ����
_`ab ��|� ���£G \] �� �x 9:�
� ñ�JË �iJ, Ã� m J� ��, ��, "
d ��W (� � ��� :�> ��|� �µP�� �
4 ��� ��PG '�ÈÉ� . �� '�ÈÉ� ASTM
d5'�É� �ú;<�, '��rG ASTM D 1559, “�
� '��¾x �:> &� ��|� \Jãä m ”6� ß
��� F (ASTM, 1994). � '���G #$��, º Ú
�, ��H, �o|9� 7�� ST d 3.1Ë Ì�, OX
� 2P� ��gq� ¥óµ� õ'�36·, ��� _
`ab ��|� ��IJ� �� ��;µÖ Ø�_`ab
�å� 7.2%~7.5%� ���� ��;< . ��� _`ab
��|� zÇ�J£[ " A���ÿ� IJ� �o: (
(2003)� ¢'�3 .
4. ������� � ��
4.1 ��� ���
� �i��G Li! ��M OW�'�, i! ��M O
� 2.1. ���� �� �����
��� ���� �� � �� ��� ��
Kirwan,Snaith,Glynn(1977)
DEFPAVNonlinea FEM, layer strain
ε: ����A: ��-����∆:��� !
"���#$%&'��
MonismithInkabi FreemeMcLean (1977)
ELSYM Layered elastic, layer strain
εzp :()����
δ(T): *+N:$%,-.�
,-/�����
�$% 0 $%12�3
Brown Bell(1979)
DEFPAV Nonlinea FEM, layer strain
q: �4 !a, b: 5�N:$%,-.�
(),-$%
��+6789 :; 5<<=
Meyer Haas(1977)
FEPAVE II FiniteElement
Layer Strain
AV: air voidT: temperatureE: error
,-/�$%
>?9 �?5<<=:@
van de Loo(1976)
BISAR elasticlayer theo.
σ : () !(103.5kPa)
��A&'��
SHELL ��BC
Kenis (1977)VESYS probabilitic
linear viselastic
e:DE$%� ��α:1-Sµ=IS/e
"�,-$%
VESYS ��BC
Francken(1977)
A,B,C,D: F!�� t: ��
/�#�$��
����GAHI
VerstraetenRomain
Veverka (1982)
Elastic layer Layer strain
Theory
A, B : F!5�C=f(Vb, Vv)E* : modulus
/�#�$��
16J ��+6KC78 :
LMN LO �P
MahboubLittle (1988)
εvp/N : visco. plasticdeform. σ: E,- !
"�&'��
εn A b∆=
εzp δ T( )Nασn 1– t[ ] σz
12--- σx σy+( )–=
επaq--- N( )b=
εp f σ1 σ3 T AV N, , , ,( ) E±=
εp CσNa=
εp N( ) εµN α–=
εp t( ) AtB C expDt 1–( )+=εp t( ) AtB=
εp t( ) At
10003--------------
B C σ1 σ3–( )
E* t1000------------
B----------------------------= =
εvp
N------- aσb=
� 3.1. �� �� � !
Q1 RSTUV
W�XY1 2 3 4 5
Z;W�
",[\] O
^\_`a O O
�6_`a O O
bW�
cd` O O O
�eO \_`a O
�eO �6_`a O
fgTh O O O O
*ij� : k lSm _`a1no #"$p BC
�24� �2D� · 2004� 3� − 3 −
W� '�, Li! $�M OW�'�, i! $�M O
W�'�, 1t�M OW�'�^ [��3�, �x ٰ�
��:��(��H " �o|9)� �}� \JjgIJ )
2�3 . � �i� �:p OW�'�44G H 4.1Ë
�, OW� '�� �}, '�n� " '�7�� d 4.1
� ¥¦�< .
4.2 ��� ����
� �i��G ���}� SÄ \Jjg IJ^ �4 �
� �M, n�, i!�M (^ j¿'�, �> 7�� O
W� '�^ [��3 . H 4.2G ��M OW�'��Ë
x Z�5 . H 4.2�� Z�� �M� �[�, n�2 �� 4.1. ��� ��""
� 4.1. ������ ��# $% �����&'
&qr�� XY
Qs$%tu
��*+ ����vwx ��vw
$%�$/ $�� $%&y
>$%&qr��
�Qs37.8oC
z��$% 0 �� 0.1kN, 300{
z$%�$, $�� :3600{, 1200{(|})
1.12kN, 3.36kN
54.4oC 0.56kN, 1.12kN
Qs37.8oC 3.36kN, 6.73kN
54.4oC 3.36kN, 6.73kN
#$%&qr��
�Qs37.8oC
z$%�$, $�� : 3600{, 1200{(|})z�$ 0 $�� : 0.2{, 0.8{
1.12kN, 3.36kN
54.4oC 0.56kN, 1.12kN
Qs37.8oC 3.36kN, 6.73kN
54.4oC 3.36kN, 6.73kN
~1$%&qr��
�Qs37.8oC
0.1kN� $% 101�$ 0 $ 2� ,-
z�$�� : 0.1, 1, 10, 100, 1000{z^$�� : 120, 120, 120, 240, 480{
1.12kN, 3.36kN
54.4oC 0.56kN, 1.12kN
Qs37.8oC 3.36kN, 6.73kN
54.4oC 3.36kN, 6.73kN
*����Ko �3O $%8 !<= : 1.12kN→ 142kPa, 3.36kN→ 428kPa, 6.73kN→ 856kPa
�� 4.2. (), *+, ,-./0 12 3�4 ��� 56
− 4 − ����� �
�^[�, Li! Bq# wN hijgå� ^ � [ F
. =>, ��HÅ º Ú�x ��> �� 3Ë �� 52
���P !� �� 2Å �� 4Z hijgå� O� e
â� �"G 'A� �×^ � [ F . �G e#> ý�
�� 9:� hijgå� O4� h?^ $^ �Ã> . �
M7�� wN cgb%#u �M7�^ i®> 6.73kN�M
� wN c�t� ë'�2 eâBq� �"& . I´,
54.4oC��� '�� '� \Jjg eâIJ^ è�6�
Z�5 .
d 4.2G �� �}� SÄ 3600K �M��Bq " �M
¢° @ 1200K(ó£ 4800K)��� OW� jgå^ Z�
5 . 'v� jgå� r�2 _`ab� ¤�JJ� �
�� zÇp jgå� O4x �Ã> .
d 4.3� �i�� �Wp \Jjg ÈPx �> �£4
56� Ø\ OW� £[x ¢ñ> ���, d 4.4G ��å
7�� SÄ \JjgÈPx �> Ø\ OW�£[ ��
(Little & Button, 1993). d 4.5G \Jjg IJ ��
OW� £[x ¥¦�< . d 4.5�� Z�� ��HÅ º
Ú�x 7��P !� _`ab ��|� OW�£[2 2
� O� OW� 4(4G 2� �) . ��HÅ º Ú�x
7�> _`ab ��|� OW� £[G Bc�6� 2�
��, OW� 4(4G 2� ¡ D^ � [ F . I´, �
� 2Š��4� wN 37.8oC '�n��� L�� �� �
�å7�� Ø\ OW�£[ �� Ù��^ � [ F . �
G ��HÅ º Ú�x ���P !� _`ab ��|�
\Jjg m J� 2� N[� G D^ ��� #$ _
`ab ��|Ë L� Õ ¯ \Jjg m J� F×^ *
> .
4.3 �� ����
H 4.3� n�, �M, i!7�� SÄ �� �}� ±�
M OW� °±^ ¥¦§ . ±�M OW� '��Ë eâp
+,� ¹_ ���}� SÄ \Jjg IJ^ L��4 µ
ø- ¤� F6¥, c��6� OW� 4(4� wN ��H
Å º Ú�x 7��P !G �� 2Å �� 4� 4(42
2� �X ¥¦Á . => �� �M6� �> +,� eâ
'A� ��HÅ º Ú�x 7��P !G ��� 7�^
> ��Z .X ¥¦Á . HW� ±�M OW� '� '
yÊ�G jgå� ±# 7�6� [�> ��M OW� '
� �Ë� ¥n jgå� 110%~180%� �� �� Ñ��
3Gé �G $Ç�M6� �� �2 ÂG k�2 �PB
q� ¸/;µ FG ��M� L� 0 � SÄ �Ë� .
� 4.2. 3� !0 12 ��� ��7
Qstu *+ $%lS1 lS2
���( 3600{) ���( 4800{) ���( 3600{) ���( 4800{)
�Qs
37.8oC1.12kN 634.00 521.47 475.08 299.22
3.36kN 2004.82(2601{)-�� 832.88 644.75
54.4oC0.56kN 443.88 323.60 470.35 389.70
1.12kN 691.38 559.26 455.58 337.90
Qs(1.41kg/cm2)
37.8oC3.36kN 855.17 736.81 683.07 598.02
6.73kN 1881.08(1300{)-�� 1098.84 936.48
54.4oC3.36kN 1253.25(1400{)-�� 877.42 775.49
6.73kN 1859.86(148{)-�� 1788.44(926{)-��
Qstu *+ $%lS3 lS4 lS5
���(3600{) ���(4800{) ���(3600{) ���(4800{) ���(3600{) ���(4800{)
�Qs
37.8oC1.12kN 497.71 348.49 389.19 247.62 505.63 340.95
3.36kN 1963.05(1202{)-�� 896.73 617.77 1271.46 981.96
54.4oC0.56kN 285.71 240.55 193.67 112.71 283.50 210.74
1.12kN 964.80 896.06 385.62 382.21 605.24 454.23
Qs(1.41kg/cm2)
37.8oC3.36kN 1033.24 911.66 528.48 426.78 1179.13 1058.74
6.73kN 2091.98(1500{)-�� 839.47 700.24 1516.41(700{)-��
54.4oC3.36kN 1000.95(480{)-�� 384.57 304.85 996.0(178{)-��
6.73kN 2174.43(84{)-�� 1082.30 904.14 1628.0(34{)-��
� 4.3. 8� ���9: ;
(Q����+
��*+
$%�$��
!(kPa)
yP�
Viljeon and meadows 1981 40oC 100 min. 207 82.7 MPa
Khedr 1986 40oC 60 min. 207 137.9 MPa
Kronfuss et al. 1984 40oC 60 min. 103 max 45.3
Lee & Lovell 1996 50oC 60 min. 827 70 MPa
� 4.4. <=7 &'0 12 8����9:
�}���
�}�>+ ESALD�&qr=�(MPa)
I �� �; �}� > 106 ESAL 51.7
II �; �}� 5*105~106 ESAL 48.3
III %� �}� 105~5*105 ESAL 34.5
IV �; �}� < 105 ESAL 20.7
�24� �2D� · 2004� 3� − 5 −
4.4 !"�� ��� �
1t�M OW� '�ÈÉ� wN, ë'�� 2�PG �
Mgq 7�� x 1 ��M OW� '�Ë ±#> 7�
�� '��X p . �MgqG VESYS(FHWA, 1978)�
�> ÈÉ^ 4K� �3 . òm, 37.8oCÅ 54.4oC� n�
�� '� ë'�� 0.1kN� ê�M6� 10t� ��MË
10t� ¢�M gq� 2z $Ç��, �@ õ�6� 0.1,
1, 10, 100, HW� 1000K ±ñ O42 Ä 42P� �
�M(0.56kN ,1.12kN, 3.36kN, 6.73kN) ����, H 9
�� 2, 2, 2, 4, HW� 8t� 'A±ñ �M^ ¢�> .
� 4.5. 3� !0 12 >*+ ���9:
lS
�Qs Qs
37.8oC 54.4oC 37.8 oC 54.4oC
1.12kN 3.36kN 0.56kN 1.12kN 3.36kN 6.73kN 3.36kN 6.73kN
1 15 - 11 14 34 - - -
2 18 30 9 18 36 45 28 -
3 18 - 16 9 25 - - -
4 25 32 25 25 55 69 74 54
5 19 23 17 16 25 - - -
- : ��� ���6 �B �@
�� 4.3. 6*+ �����?@
�� 4.4. A,��B(Cp)@ *+�D
�� 4.5. EF*+ ����� ?@
− 6 − ����� �
HW� ¥� ��� �M ¢�2 2¥G �t�� hijg
�(εp) ���X p . �3X i> hijg�(εp)Ë �M
'A(sec) �H`4#� �W��, H 4.4Š� �]>
j[�^ ��> . \Jjg -�� εp(N) = µεN−α á^ �
:�3 . �4�, hijg�(εp), rå��$Ç ö[(N), µÅ αG hijg�� j[� . HW� ε� 10K� P!�
M� '�;G ¤�� 0.03K ±ñ� jg�� . � á�
hijg� j[x �:�� rå��$Ç ö[� SÄ h
ijg�^ iÕ [ FG �[� iJ;µF . H 4.5G
1t�M OW� '�6��/ ¥n 'A-jgå +£x Z
�o�, d 4.6� VESYSÈÉ� �� ��;µÖ \Jjg
IJ� +,p ��j[÷^ ¥¦�< . d 4.5�� �µÖ�� 4.6. G7HIJ:0 12 3�4 A,��B
� 4.6. VESYS K�0 �% LM �:
F!�� I S � � �
lS1
37.8+
�Qs1.12kN 0.00053 0.233 27.62259 0.767 0.0000044
3.36kN 0.00234 0.210 56.98042 0.790 0.0000086
Qs3.36kN 0.00353 0.143 63.18239 0.857 0.0000080
6.73kN 0.00592 0.136 93.46843 0.864 0.0000086
54.4+
�Qs0.56kN 0.00052 0.191 12.30671 0.809 0.0000080
1.12kN 0.00213 0.119 80.20590 0.881 0.0000032
Qs3.36kN 0.00374 0.134 45.58127 0.866 0.0000110
6.73kN 0.00623 0.160 150.88447 0.840 0.0000066
lS2
37.8+
�Qs1.12kN 0.00137 0.165 52.26783 0.835 0.0000043
3.36kN 0.00279 0.145 45.39070 0.855 0.0000089
Qs3.36kN 0.00303 0.120 39.95807 0.880 0.0000091
6.73kN 0.00470 0.120 94.64638 0.880 0.0000060
54.4+
�Qs0.56kN 0.00056 0.158 18.21648 0.842 0.0000048
1.12kN 0.00218 0.094 61.96675 0.906 0.0000033
Qs3.36kN 0.00472 0.089 98.89195 0.911 0.0000043
6.73kN 0.00704 0.102 57.69245 0.898 0.0000124
lS3
37.8+
�Qs1.12kN 0.00097 0.190 35.23493 0.810 0.0000052
3.36kN 0.00258 0.179 64.35776 0.821 0.0000072
Qs3.36kN 0.00426 0.134 59.74638 0.866 0.0000096
6.73kN 0.00550 0.157 78.09262 0.843 0.0000111
54.4+
�Qs0.56kN 0.00073 0.175 25.92017 0.825 0.0000050
1.12kN 0.00249 0.122 76.56680 0.878 0.0000040
Qs3.36kN 0.00482 0.162 53.18612 0.838 0.0000147
6.73kN 0.00758 0.196 94.98157 0.804 0.0000156
lS4
37.8+
�Qs1.12kN 0.00108 0.112 54.16030 0.888 0.0000022
3.36kN 0.00380 0.083 60.79231 0.918 0.0000052
Qs3.36kN 0.00338 0.074 97.62604 0.926 0.0000025
6.73kN 0.00289 0.108 111.45137 0.892 0.0000028
54.4+
�Qs0.56kN 0.00020 0.172 3.94627 0.828 0.0000088
1.12kN 0.00189 0.085 60.52618 0.915 0.0000027
Qs3.36kN 0.00302 0.064 60.07252 0.936 0.0000032
6.73kN 0.00409 0.105 50.43760 0.895 0.0000085
lS5
37.8+
�Qs1.12kN 0.00097 0.161 40.70184 0.839 0.0000038
3.36kN 0.00202 0.187 58.93161 0.813 0.0000064
Qs3.36kN 0.00215 0.159 71.31754 0.841 0.0000048
6.73kN 0.00290 0.181 91.50962 0.819 0.0000057
54.4+
�Qs0.56kN 0.00026 0.185 11.09791 0.815 0.0000044
1.12kN 0.00166 0.123 88.99729 0.877 0.0000023
Qs3.36kN 0.00301 0.155 59.19253 0.845 0.0000079
6.73kN 0.00617 0.169 114.79560 0.831 0.0000091
�24� �2D� · 2004� 3� − 7 −
4
4
4
4
4
4
4
4
4
3
3
4
4
4
4
4
4
��j[÷^ 5� á� c��� £.p rå$Çö[� c
> hijg�^ H 4.6� ¥¦�< . ��HÅ º Ú�
� 7�� ÏG �� 2Å �� 4� hijg�� 2� �
X ¥66·, H M��� ����H _`ab ��|� \
Jjg m J� 2� N[> D6� ¥¦Á .
5. KENLAYER !"# $%&��
5.1 #$%& �'()
Burmister� ��J�í� 0b7 4É6� �8;� 9
:/� yÆË �; ��J�í� º<^ = �.��H
�� ¹� vy;µ _`ab ��i7�� i7��� 9
:;� F . ��J�í^ 2� òm �.¿�� ��i
7��� 9:p �.��H�� 1963� Chevron �i\�
� vyp CHEV ��H�� . 1973�� Shell �V9��
vyp BISAR ��H�� 2� Zî�6� 9:;G ��
J�� �.��H�6� ��i7��� ì�Ë jg>^
2� �³�X iÕ [ FG Ç?> [½� ÚÛ^ ���
� Fµ Ä ��J��H�^ L��G 456� 9:;
� F . Ãë@è�� vyp WESLEA ��H�� \g9
:/�� Z Ó��6� 9:;·, Ä ��H�� L�
û!�X [�p . 1986�� Finn (� _`ab ��i7
��� k�*lË ºA�BÞ(rutting) -�Õ [ F�
� ��J�í� �� ì�[5� SÄ |J(Stress-
dependent Property)� L²g^ �:> �.��H��
PDMAP vy�3 . => Kenturky c½�� vyp
KENLAYER ��H�� ���� c�� ²g�J, L²
g�J, =G ¤�J��� 2{�·, ��M =G �±�M
� c��� ��� 2{> ��i7����H�� . �G
k�*lË ºACBÞ� c> fB��(Damage Analysis)
� [�Õ [ F�� ;µ F . ��i7���^ ���
��J�í� º<^ = �.��H�÷� ¹� vy;µ
9:;� F (���, 2002).
5.2 KENLAYER #$ ��
� �i��G �J��� _`ab ���� �£[à -
� 4É� Damage Analysis ÈÉ^ [��3� 1t�M
OW� '� �Ë��/ �µÖ OW� £[� &[�
Creep compliancex �� �� 7�� $h�3 . => 1
t�M OW� '�� jgåË L��4 �� _`ab d
�� ';x 65mm� �# 'D6·, d�� ';� SÄ
[à ��+£x ßà�4 �� 65mm�� 203mmEP ¥
óµ� õ'�3 . HW� UB " 4�� |J¾ j¿�
SÄ h?� � �� 7�� $h�3 .
F ��� iJ : 3� i7(_`ab d�, 4�, UB)
F ��� ��n� : 37.8oC(100F)
F �A ��� )*n� : 25oC(77F)
F '; : 1t�M OW� '�: ë'� ';� 65mm
�/ 203.2mmEP
F �M(�P¸) 7� : 3.36kN(i!)(=60.15psi), $w
- 154mm
F �J£[ : 4�(206,850kPa), UB(103,425kPa)
F ��å : 500z/#, 182500z/�
F �� �} : 5v
5.3 KENLAYER #$*+
d 5.1� KENLAYER ��H���� �:p _`ab
��| �}� �M'A� SÄ creep compliancex Z�5
. VESYS ���ËÅ� L�x �� 1t�M OW�'�
���/ creep compliancex ���3 . d 5.2G _`
ab ��| �}� ��� d� '; j¿� �> G å
� 5.1. ��0 NOP �� �� 4 Creep Compliance
��({)Creep Compliance (kPa)
lS 1 lS 2 lS 3 lS 4 lS 5
0.001 2.058E-04 1.806E-04 2.452E-04 2.903E-04 1.152E-0
0.003 2.408E-04 2.060E-04 2.843E-04 3.147E-04 1.371E-0
0.01 2.859E-04 2.381E-04 3.342E-04 3.439E-04 1.660E-0
0.03 3.344E-04 2.716E-04 3.873E-04 3.729E-04 1.976E-0
0.1 3.971E-04 3.138E-04 4.554E-04 4.074E-04 2.392E-0
1 5.516E-04 4.137E-04 6.206E-04 4.827E-04 3.448E-0
10 7.662E-04 5.454E-04 8.456E-04 5.718E-04 4.968E-0
100 1.064E-03 7.189E-04 1.152E-03 6.774E-04 7.160E-0
500 1.339E-03 8.721E-04 1.431E-03 7.626E-04 9.243E-0
1000 1.478E-03 9.477E-04 1.570E-03 8.025E-04 1.032E-0
1600 1.581E-03 1.003E-03 1.673E-03 8.307E-04 1.112E-0
� 5.2. QRST0 12 �� 4 UV7(m), WR��B X YZ:[(\)
��(mm)37.8 oC (���))
lS 1 lS 2 lS 3 lS 4 lS 5
65.0 0.566 0.564 0.569 0.569 0.556
101.6 0.513 0.505 0.516 0.518 0.493
127.0 0.475 0.465 0.480 0.483 0.455
152.4 0.439 0.429 0.447 0.447 0.417
177.8 0.409 0.399 0.414 0.417 0.384
203.2 0.381 0.371 0.386 0.386 0.356
��(mm)37.8 oC (�����,strain)
lS 1 lS 2 lS 3 lS 4 lS 5
65.0 -2.12E-04 -2.22E-04 -2.01E-04 -1.96E-04 -2.53E-0
101.6 -3.52E-04 -3.58E-04 -3.46E-04 -3.45E-04 -3.64E-0
127.0 -3.80E-04 -3.79E-04 -3.79E-04 -3.79E-04 -3.75E-0
152.4 -3.74E-04 -3.69E-04 -3.76E-04 -3.77E-04 -3.60E-0
177.8 -3.51E-04 -3.44E-04 -3.55E-04 -3.56E-04 -3.32E-0
203.2 -3.22E-04 -3.14E-04 -3.25E-04 -3.27E-04 -3.00E-0
��(mm)37.8 oC (���, �)
lS 1 lS 2 lS 3 lS 4 lS 5
65.0 4.38 4.49 4.25 4.19 4.93
101.6 7.93 8.55 7.57 7.49 9.48
127.0 11.8 10.68 11.15 11.01 8.84
152.4 13.41 11.66 14.86 15.27 10.15
177.8 16.49 14.69 18.03 18.45 13.22
203.2 22.12 20.02 23.93 24.42 18.4
− 8 − ����� �
n,
-
a-
te,
e
lt
m,
d
ge
Ë ��� ��� yÊ�G ��jg�^ Z�5 . ���
Ë��/ ��p G å " ��jg��� ���� ';
� ST \ ¼ª�X j�3 . Q, KENLAYER�
Damage Analysis �� ' -�[à� ���� �:�G
G åË ��� ����/ yÊ�G ��ì�Ë H:�Ë
� L��� .Ip . ST�, èü´ hijgå� O4�
ST _`ab ��|� IJ^ Jè�4G \ µø- D
6� Jèp . ��H�� ���� Î [ F��, ��p
�Ë��/ �µPG ���� G å, ��jg� " -�
[à� creep compliance� ¼ª�X j�^ � [ F .
�D� ��H� ��^ �> ���� ���� ��j[
� M]J^ �Ã�G D6�, OW� '�� d5¿ ���
7!´ ��W;µ¶ Õ D� .
6. �' � ()��
PKEP [�p ��:��x �:> _`ab ��|�
\Jjg IJ)2'��Ë��/ ×Ë Ì� �í^ �I
�3 .
•_`ab ��|� \JjgIJ^ )2�4 �� �
> �}� OW�'�^ [��3 . '�7�� i!�M�
��, n�j¿, �M� �} (^ ��´ 7��� �:�
3 . ��MOW�'�� wN �� 2(¢ÿ��H ��|),
�� 4(����H ��|)� hijgå� Ä ��|�
L� �X ¥¦Á . �u> ÓËG 54oC��� '��Ë�
� L» à³�X ¥¦Á .
•PKEP ydp '�7�� SÄ Ø\OW�£[x L
�> �Ë, '�7��� �A� r�2 Fµ Ý��� L�
G Õ [ ÏPQ, A��� L�x �3 . i!�M^ 2�
P !� ��|� wN �u �i2 ¢'> 45��
\ ÃÆ�G D6� )2;<�, i!�M^ �:> wN ¢
ÿ��H ��|Ë ����H ��|� 45� Ù�> �
^ ¥¦�< . õ�� n�, �M�} " �M��'A� r
�� �> ��� ��J��x ���4�G \ �W
2 F6¥, )2p x Ù°� JèÕ ¯, ¢ÿ��H �
�|� Mt> \Jjgm J^ 2PG D6� Jèp .
•rå�M^ Ú9> ±�M OW�'�^ [��3 . '
��Ë, ¢ÿ��H ��| " ����H ��|^ ¢ï>
¥NP ��|� \Jjg =G eâBq� �"& . I´,
��M��' µG �� \Jjg� c> m J^ Z�5
��| &' ¡ \Jjg " eâBq� �Æ> D6� Î
¯, \Jjg IJ)2' ±�M^ �:�G D� ®�7�
^ L» �®Õ [ FG ÈÉ�«�, �x $h> '�^
��¶ Õ D� . =>, i!�M� SÄ \JjgIJ� O
X ÆTP«�, ®�7�^ �®�G i!�M� $O' '
�� �:;µ¶ Õ D� .
• VESYS ÈÉ^ �:> 1t�MOW� '�^ [��3
�, '��Ë��/ rå$Çö[� SÄ ���� hijg
å^ -��3 . -�p hijgå^ 456� Î ¯, ¢
ÿ��H ��|Ë ����H ��|� hijgå� �X
¥¦Á�, Ä ��|� �Z \ OX ¥¦Á . �u
> r�G �� '�n� " i!�M^ �:> wN� O
X yÊ> D6� ÃPµ Î ¯, ���� hijgå -�
� Fµ� �� |J^ ���G '�n� " i!�M�
0N M]> �� Jè;�, $O' �:��¶ Õ D� .
• KENLAYER ��J ��H�^ �:�� ì�-jgI
J^ )2�3�, Damage Analysisx �:�� ����
ýÑ[à^ )2�3 . ����G ��� \JjgË d�
� ��� y�G ��*l� M]> ]\��, ��
�� èü \JjgQ^ �ø> ��� �ËÅG \ B�
> �Ë2 ¥¦Á . �G ��*l� �> ÓË2 $hp
D^ �Ã> . ���Ëx 4K� Î ¯, ����H ��
|� ¢ÿ��H ��|� L� \ ��> �Ëx ¥¦�
< .
*+� ,
� �iG >�˽�è Q�4K�i(Ë¢R� 2000-2-
31100-001-2) P86� [�;<�, �� ª9O8S .
-./0
w��}u(2002) ��� ����� � ��� �����(���� ����� ), 1�= 14�+ DX���,KPRP-G-02.
�� , ¡¢£, ¤�/(2002) ,-&qr��o BCO ¥¦§¨2�� ���� �© �=yP J�, ������ ���,22ª, 1-DV, pp. 71-80
¡¢£, B<V(1997) �(�+6«� f�¬(Waste Material) C �¢, �������, ",yh, pp. 76-86.
®gC, v�¯, B<V(2003) _`a9 fgTh° BCO ¥¦§¨ RST� ����±�m <O (Q, �� !"��,Vol. 20, No. 2, pp. 186-192
®gC, B<V, v�¯(2002) ¥¦§¨ 2�C �²W�6� _`a9 fgTh� T�HI (Q, �� !"���, 19ª 5V, pp. 511-517
Emery, J. J. (1982) Slag Utilization in Pavement ConstructioExtending Aggregate Resources, ASTM STP 774, AmericanSociety for Testing Materials, pp. 95-118.
Hicks, R. G. (1988) State-of-the-Art on Rutting in Asphalt Concrete, Proceedings, Third IRF Middle East Regional Meeting,Vol. 6, 6.119-6.144
Little, D.N. and J.W. Button (1993) Development of Criteria toEvaluate Unaxial Creep Date and Asphalt Concrete Permnent Deformation Potential, TRR, No. 1416, pp. 1-10
Khedr, S. A. (1986) Deformation Mechanism in Asphalt ConcreJournal of Transportation Engineering, ASCE, Vol. 112, No. 1,pp. 29-45
Lee, K. (1996) The Use of Waste Materials (Air-Cooled FurnacSlag and Pyrolyzed Carbon Black) in Hot Mix Asphalt, Ph.DThesis, Purdue University, W. Lafayette, Indiana.
SHRP (1994) Stage I Validation of Relationship Between AsphaProperties and Asphalt Aggregate Mix Performance, ReportNo. SHRP-A-398, Strategic Highway Reseach PrograNational Research Council, Washington, D. C.
Uzan, J. (1982) Permanent Deformation in Pavement Design anEvaluation, Technion, Israel Institute of Technology.
van de Loo, P. J. (1974) Creep Testing : A Simple Tool to JudAsphalt Mix Stability, Proceedings, AAPT, Vol. 43, pp. 253-284
(³�": / h": / hµ�": )